**Filled Holes on Skin**

Feature holes in a skin are filled in with cured resin during printing.



:::

:::VerticalSplitItem
::Image[]{src="https://api.archbee.com/api/optimize/3CesIL2dYMCHPZvRjp8S0/rqsPCi9vGSZwOiscfK5vN_image.png" size="80" width="600" height="600" position="center" alt="Filled Holes on Skin" showCaption="false"}
:::
::::

# How to Identify

Skins are the name for a thin, solid covering over a lattice. Holes are sometimes designed into the skin as a design feature and/or for drainage of resin.

Filled Holes on Skin can be diagnosed as follows:

- Holes appear as dimples rather than openings.

How to differentiate from similar appearing defects:

- [Overcure](docId\:X2fADtb4J-LqyUErv3Dgh) may appear similar for small holes. The difference will be that overcure will occur equally in all holes printed in the XY plane in most cases, whereas filled holes on skin may only occur in some holes in the XY plane, particularly holes near the center of the part.
- [Excess Resin](docId\:yrPf8M5sTjm3dFCE-WwKX) may appear similar for small holes. The difference will be that excess resin in the holes will have a shinier surface finish than the skin around it, due to curing after printing rather than during.

::::LinkArray
:::LinkArrayItem{headerType="IMAGE" headerImage="https://api.archbee.com/api/optimize/Nvx7WdIjE2XFpMaBlbCES-QeuzePWsz_gUlhDFa-Ihc-20240729-203639.jpg"}
**Cause** - <font color="#d32f4a">**Poor Resin Flow**</font>

**Solution** - Print Preparation or Part Design
:::
::::

# Troubleshooting

:::hint{type="info"}
It is recommended that you review all the possible solutions before taking action to ensure you are pursuing the best course of action.
:::

If the best course of action is not apparent, try the troubleshooting options in the order listed. Refer [here](docId\:pPm8gmeGCY_0fkFwgTCyj) for more tips.

## Print Preparation or Part Design Adjustments

The following solutions will address print or part-related causes of the defects. Choose among the suggested actions below and select the best approach for your application. Usually only one type of adjustment is needed.

:::::ExpandableHeading
### Orientation

::::VerticalSplit{layout="left"}
:::VerticalSplitItem
Reorient the part so the skin and holes are oriented vertically instead of in the XY plane.
:::

:::VerticalSplitItem
![Orientation](https://api.archbee.com/api/optimize/3CesIL2dYMCHPZvRjp8S0/KZYW9IpITV-R4_XXzhxLG_image.png)
:::
::::
:::::

:::::ExpandableHeading
### Design

::::VerticalSplit{layout="left"}
:::VerticalSplitItem
Increase hole diameter by 25%.
:::

:::VerticalSplitItem
![Design](https://api.archbee.com/api/optimize/3CesIL2dYMCHPZvRjp8S0/CeYYH8sRWYLfBXv6b8lH__3fnlh2mu4j8i5ovk-63pbqrcfatxypy9d.gif)
:::
::::
:::::

:::ExpandableHeading
### Print Plan Adjustments

Reference [Print Plan Adjustments](docId\:NxUK0dltz_vemEAU0DIpN) for guidance on the following parameters:

[4 Settle Down Parameters](docId\:nnb8zuqLpvpRucPpbWwsR)&#x20;

- *Delay Timing Parameters*
  - Minimum Pre-Exposure Delay
  - Minimum Time Force Slope Down Settled
:::

:::hint{type="info"}
If problems persist, please reach out to [Carbon Support](mailto\:support@carbon3d.com).
:::

# Explanation & Causes

## Explanation

During the settle down phase of printing a slice, <font color="#9393fc">**resin is flowing out from under the part**</font>. At the same time, oxygen is recharging after printing the previous slice. As the oxygen recharges, you can picture this as the slice image getting increasingly less blurry. At full charge, the contrast in the slice image is at its full clarity.

::::VerticalSplit{layout="middle"}
:::VerticalSplitItem
The filled holes on skin defect occurs when the settle down phase is moving too quickly for the resin flow and oxygen recharge to have reached its optimal printing condition before <font color="#6752ff">**curing the slice.**</font>

Reference [DLS Printer Dynamics](docId\:U7XYytjyDp3BvsYy2qKcU) for more information on the phases of printing a slice.
:::

:::VerticalSplitItem
![Filled holes on skin](https://api.archbee.com/api/optimize/3CesIL2dYMCHPZvRjp8S0/eJpb3Psygp9oqY_B0m236_image.png)
:::
::::

Refer to the animations below to see a magnified view of how this hole appears during the settle down phase under both <font color="#d32f4a">**bad**</font> and <font color="#30c49a">**good**</font> conditions.

::::VerticalSplit{layout="middle"}
:::VerticalSplitItem
![Bad condition](https://res.cloudinary.com/carbon3d/image/upload/Education/Troubleshooting/Part-Defects/Filled-Holes-on-Skin/Filled-holes-bad-gif.gif)

<font color="#d32f4a">**Defect occurs**</font> when the settle down phase is too fast for proper <font color="#9393fc">**resin flow**</font> and to recharge the oxygen for full clarity in the slice before <font color="#6550ff">**curing**</font>.
:::

:::VerticalSplitItem
![Good condition](https://res.cloudinary.com/carbon3d/image/upload/Education/Troubleshooting/Part-Defects/Filled-Holes-on-Skin/Filled-holes-good-gif.gif)

The <font color="#32c49a">**hole prints as expected**</font> when the settle down phase is long enough for proper <font color="#9393fc">**resin flow**</font> and oxygen recharge to reach full clarity in the slice upon <font color="#6550ff">**curing**</font>.
:::
::::

## Causes

### Print Preparation or Part Design

::::VerticalSplit{layout="middle"}
:::VerticalSplitItem
How the part is **oriented**, **supported**, or **designed&#x20;**&#x69;s causing the defect.
:::

:::VerticalSplitItem
![Print Preparation or Part Design Cause](https://api.archbee.com/api/optimize/3CesIL2dYMCHPZvRjp8S0/LhaBjVT_Yxhp03FPtHLyF_orient-and-support-quick-view-v0101-xxs.gif)
:::
::::

| Root Issue | Problem                                                          | Why Defect Presents                                                                                                                           |
| ---------- | ---------------------------------------------------------------- | --------------------------------------------------------------------------------------------------------------------------------------------- |
| Oriented   | The skin and holes are oriented in the XY plane during printing. | The settle down phase needs to be longer for the resin to flow properly across a large cross section parallel to the window.                  |
| Designed   | The holes are too small.                                         | If the settle down phase needs to be made too long for an efficient production printing time, the holes can be designed larger to compensate. |

### Print Plan Adjustments

::::VerticalSplit{layout="middle"}
:::VerticalSplitItem
![Print Plan Adjustments](https://api.archbee.com/api/optimize/3CesIL2dYMCHPZvRjp8S0/BzaP59syjyUMWREOHSLmE_print-plan-adjustments-v142.png)
:::

:::VerticalSplitItem
[Print Plan Adjustments](docId\:NxUK0dltz_vemEAU0DIpN) adjust the print plan to optimize mid to high volume production and/or address part defects.&#x20;

In doing so, adjustment may both **prevent or cause defects**. Below are adjustments that can cause this defect.
:::
::::

| Printing Stage | Parameter Type | Type of Adjustment                        | Why Defect Presents                                                          |
| -------------- | -------------- | ----------------------------------------- | ---------------------------------------------------------------------------- |
| 4 Settle Down  | Delay Timing   | <font color="#ff3399">**Decrease**</font> | The settle down phase is too fast for proper resin flow and oxygen recharge. |